當(dāng)前位置:首頁-新聞中心-行業(yè)資訊注塑模具表面縮水如何?

注塑模具表面縮水如何?

來源:http://www.qixunbaba.com/ 日期:2022-03-18

在生產(chǎn)中注塑模具制品表面經(jīng)常會出現(xiàn)很多的缺陷,如飛邊,缺膠,縮水,氣溫,發(fā)白,氣泡,料發(fā)等等。要這些問題,要知道是什么原因產(chǎn)生。
In production, many defects often appear on the surface of injection mold products, such as flash, lack of glue, shrinkage, temperature, whitening, bubbles, material hair and so on. To solve these problems, we must first know what causes them.
生產(chǎn)中注塑模具制品表面出現(xiàn)縮水如何?縮水也稱為凹陷,縮痕,是指表面不平整,注塑模具制品由內(nèi)產(chǎn)生淺坑或者是凹窩。注塑模具制品縮水的原因大概分為兩大問題。
How to solve the shrinkage on the surface of injection mold products in production? Shrinkage, also known as depression and shrinkage mark, refers to the uneven surface and shallow pits or pits produced in the injection mold products. The reasons for the shrinkage of injection mold products can be divided into two major problems.
1.注塑模具問題 有可能是模具的澆口及流道截面積過小,如果是這樣就要擴(kuò)大相應(yīng)位置的截面積。也有可能是排氣不良,針對其問題,可以改善排氣系統(tǒng)。再有就是冷卻系統(tǒng)設(shè)計(jì)不合理,冷卻不均勻冷卻不足,可以改善冷卻系統(tǒng)。
1. The problem of injection mold may be that the cross-sectional area of the gate and runner of the mold is too small. If so, it is necessary to expand the cross-sectional area of the corresponding position. There may also be poor exhaust. Aiming at the problem, the exhaust system can be improved. Another is the unreasonable design of the cooling system, uneven cooling and insufficient cooling, which can improve the cooling system.
2.注塑工藝調(diào)機(jī)問題。有可能注塑壓力太低和注塑速度太慢,可以適當(dāng)加大注射壓力和提高注射速度?;蛘呤潜簳r間太短,可以適當(dāng)合理控制保壓時間。
2. Adjustment of injection molding process. It is possible that the injection pressure is too low and the injection speed is too slow. You can appropriately increase the injection pressure and speed. Or the pressure holding time is too short, so the pressure holding time can be properly and reasonably controlled.
總之注塑模具制品表面出現(xiàn)縮水或者是其它什么問題,先要找出它產(chǎn)生的原因,再根據(jù)原因找出相應(yīng)的方法,對癥下藥。
In short, in case of shrinkage or other problems on the surface of injection mold products, we should first find out the causes, and then find out the corresponding solutions according to the causes.
立強(qiáng)模具(http://www.qixunbaba.com)現(xiàn)擁有精密的微電腦注塑機(jī)47余臺,年生產(chǎn)能力達(dá)5000噸;擁有精密無塵噴涂生產(chǎn)線六條,可為客戶提供各種顏色的單色或套色噴涂業(yè)務(wù),濟(jì)南注塑加工并能進(jìn)行表面處理及絲網(wǎng)漏印、燙印服務(wù)。
Liqiang mould( http://www.qixunbaba.com )Now it has more than 47 precision microcomputer injection molding machines, with an annual production capacity of 5000 tons; It has six precision dust-free spraying production lines, which can provide customers with monochrome or chromatic spraying business of various colors, Jinan injection molding processing, surface treatment, screen missing printing and hot stamping services.

相關(guān)產(chǎn)品 / Related products

濟(jì)南立強(qiáng)模具有限公司

魯ICP備15002024號-2

網(wǎng)站地圖    TXT    XML
嘉义县| 静海县| 青川县| 陇西县| 阳春市| 平邑县| 历史| 柘城县| 宿州市| 大庆市| 黑山县| 博乐市| 扬中市| 广德县| 武冈市| 潍坊市| 府谷县| 纳雍县| 桂东县| 海门市| 海城市| 白玉县| 行唐县| 固镇县| 天全县| 新昌县| 陈巴尔虎旗| 漠河县| 澜沧| 合江县| 逊克县| 南漳县| 荥经县| 平舆县| 视频| 靖宇县| 额尔古纳市| 丹凤县| 龙胜| 东明县| 武冈市|